Refractory Library
Magnesia carbon bricks for EAF, BOF converters and steel ladles
Grades by furnace zone, with full chemistry and physical data. Selected, checked and supplied from China by GZ Visions, Shanghai.
Quick answer
Magnesia carbon (MgO-C) bricks are the standard working lining for electric arc furnaces, BOF converters and steel ladles. GZ Visions in Shanghai supplies them by zone, from bath and bottom to slag line, hot spots, trunnions and tap holes, with MgO from 72 to 83% and fixed carbon from 10 to 16%.
The material
What a magnesia carbon brick is
A magnesia carbon brick combines high purity magnesia (MgO) with graphite, usually bonded with resin. Magnesia resists the basic slag of steelmaking. Graphite is not wetted by slag and conducts heat, which gives the brick its resistance to slag penetration and to thermal shock. Metallic antioxidants protect the graphite where air and oxidising slag reach the hot face.
More graphite means better thermal shock and slag penetration resistance, so the slag line, hot spots and trunnions use grades with 14 to 16% fixed carbon. Less graphite means higher density and strength, so the bath, bottom and impact zones use grades with 10 to 12%. Zones exposed to oxidation and abrasion use grades with a higher hot modulus of rupture.
How to read the tables: MgO and fixed carbon in % (minimum), apparent porosity in % (maximum), bulk density in g/cm³ (minimum), cold crushing strength (CCS) in MPa (minimum), hot modulus of rupture (HMOR) at 1400 °C after 30 minutes in MPa (minimum). These are specification limits, not averages. GZ grade codes are GZ Visions designations. Each specification is listed once: where several supplier variants share identical figures, they appear under one GZ code.
Electric arc furnace
EAF magnesia carbon grades by zone
Bath
Lower sidewall and bath area under the slag line.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-E01 | 83 | 10 | 4 | 3.02 | 40 | 6 |
| GZ MC-E02 | 79 | 14 | 3 | 2.98 | 35 | 6 |
Slag line and hot spots
The zones that see slag attack and arc flare. All grades here have a hot modulus of rupture of 10 MPa.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-E03 | 80 | 10 | 4 | 3.02 | 40 | 10 |
| GZ MC-E04 | 78 | 12 | 4 | 3.00 | 40 | 10 |
| GZ MC-E05 | 76 | 14 | 3 | 2.98 | 35 | 10 |
| GZ MC-E06 | 74 | 16 | 3 | 2.96 | 35 | 10 |
EBT tap hole sleeve
Sleeve bricks of the eccentric bottom tapping channel.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-E04 | 78 | 12 | 4 | 3.00 | 40 | 10 |
| GZ MC-E05 | 76 | 14 | 3 | 2.98 | 35 | 10 |
EBT seating block
The block around the tap hole at the furnace bottom.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-E03 | 80 | 10 | 4 | 3.02 | 40 | 10 |
| GZ MC-E04 | 78 | 12 | 4 | 3.00 | 40 | 10 |
BOF converter and refining ladle
Converter magnesia carbon grades by zone
Bath and bottom
Molten bath area and bottom of the vessel.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-L01 | 83 | 10 | 4 | 3.00 | 40 | 6 |
| GZ MC-L02 | 81 | 12 | 4 | 2.98 | 40 | 6 |
| GZ MC-L03 | 79 | 14 | 3 | 2.96 | 35 | 6 |
| GZ MC-L04 | 83 | 10 | 4 | 3.02 | 40 | 6 |
| GZ MC-L05 | 81 | 12 | 4 | 3.00 | 40 | 6 |
| GZ MC-L06 | 79 | 14 | 3 | 2.98 | 35 | 6 |
Barrel and impact face
Vessel body and the face hit by scrap and hot metal at charging.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-L07 | 80 | 10 | 4 | 3.02 | 40 | 10 |
| GZ MC-L08 | 78 | 12 | 4 | 3.00 | 40 | 10 |
Slag line and trunnion
The highest wear zones: slag line and the trunnion area.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-L09 | 76 | 14 | 3 | 2.98 | 40 | 10 |
| GZ MC-L10 | 76 | 14 | 3 | 2.98 | 35 | 10 |
| GZ MC-L11 | 74 | 16 | 3 | 2.96 | 35 | 10 |
Tap hole area
Bricks around the steel tapping hole.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-L08 | 78 | 12 | 4 | 3.00 | 40 | 10 |
| GZ MC-L10 | 76 | 14 | 3 | 2.98 | 35 | 10 |
| GZ MC-L12 | 74 | 12 | 4 | 3.00 | 40 | 10 |
| GZ MC-L13 | 72 | 14 | 3 | 2.98 | 35 | 10 |
Cone
Upper cone (furnace cover) of the vessel.
| GZ grade | MgO % min | Fixed C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ MC-L08 | 78 | 12 | 4 | 3.00 | 40 | 10 |
| GZ MC-L10 | 76 | 14 | 3 | 2.98 | 35 | 10 |
Steel ladle
Alumina magnesia carbon bricks for ladle wall and bottom
For the wall and bottom of steel ladles. Alumina and magnesia react in service to form spinel, which tightens joints and resists slag, with less carbon than a magnesia carbon brick.
| GZ grade | Al₂O₃ % | MgO % | C % | Porosity % max | Density g/cm³ min | CCS MPa min |
|---|---|---|---|---|---|---|
| GZ AMC-01 | 82 | 10 | 2 | 10 | 3.30 | 45 |
| GZ AMC-02 | 60 | 20 | 7 | 6 | 3.19 | 40 |
| GZ AMC-03 | 52 | 38 | 10 | 10 | 3.15 | 40 |
| GZ AMC-04 | 65 | 10 | 7 | 8 | 2.95 | 50 |
| GZ AMC-05 | 68 | 10 | 7 | 7 | 3.00 | 50 |
Converter tapping
Monoblock tap hole bricks
One piece tap hole bricks for converters: no joints along the tapping channel.
| GZ grade | MgO % min | C % min | Porosity % max | Density g/cm³ min | CCS MPa min | HMOR MPa min |
|---|---|---|---|---|---|---|
| GZ TH-01 | 78 | 10 | 4 | 2.92 | 40 | 8 |
| GZ TH-02 | 80 | 14 | 4 | 2.90 | 40 | 10 |
HMOR for monoblocks measured at 1400 °C after 0.5 hours.
How we work
What GZ Visions does for your order
- 01We match GZ grades to your furnace, your zones and your lining drawing or brick list.
- 02We quote by zone and by tonne, FOB China or delivered to your port.
- 03We check the order at the factory before it ships and can arrange third party testing at your request.
- 04One contract and one point of contact at GZ Visions.
- 05Languages: English, Turkish, Portuguese and German from Cengiz; Arabic, Spanish and Chinese through our team.
FAQ
Frequently Asked Questions
- What is a magnesia carbon brick used for?
- It is the working lining of steelmaking vessels: electric arc furnaces, BOF converters and steel ladles. High purity magnesia resists basic slag, and graphite gives resistance to slag penetration and thermal shock, so the brick survives repeated heats at steelmaking temperatures.
- Which magnesia carbon grade goes in the EAF slag line?
- The slag line and hot spots use grades with MgO from 74 to 80%, fixed carbon from 10 to 16% and a hot modulus of rupture of 10 MPa at 1400 °C. Higher carbon helps where thermal shock and slag penetration are severe. We match the grade to your slag, your practice and your lining drawing.
- What is the difference between magnesia carbon and alumina magnesia carbon bricks?
- Magnesia carbon bricks are based on MgO and are used in the hottest, most basic zones. Alumina magnesia carbon bricks combine alumina and magnesia with less carbon and are used in steel ladle walls and bottoms, where alumina and magnesia react in service to form spinel and tighten the lining.
- Do you supply tap hole bricks for converters?
- Yes. One piece monoblock tap hole bricks with MgO of 78 or 80% and carbon of 10 or 14%, and magnesia carbon bricks for the tap hole area of the vessel. EAF tap hole sleeve and seating block grades are listed separately.
- How do I get a quote?
- Send the furnace type and size, the zones or your brick list or lining drawing, quantities in tonnes and your destination port. A person from GZ Visions replies the same business day with matching GZ grades and the next questions.
Request a quote
Send your brick list or lining drawing.
Furnace type and size, zones, quantities in tonnes and destination port. A person replies the same business day.