    Two datasheets can look the same and describe two very different bricks. A buyer's guide from GZ Visions, Shanghai.

    Quick answer

    Read the label before the number. Every value on a refractory datasheet is a guaranteed minimum, a guaranteed maximum or a typical value, and it only means something with its test condition: temperature, load and time. For a lining that carries load, refractoriness under load and creep at your working temperature matter more than refractoriness or cold strength. Ask for guaranteed limits and the test standard, then have the shipment tested against them.

    Read the label first

    Every number has a type and a condition

    A value on a datasheet is one of three things. A guaranteed minimum, such as Al₂O₃ 75%, means no brick in the order should test below it. A guaranteed maximum, such as porosity 20%, means none should test above it. A typical value is an average, often from the best batches, and guarantees nothing.

    Then look for the condition. Strength after drying is not strength after firing. Creep at 1300 °C is not creep at 1400 °C. A number without its temperature, load or test time cannot be compared with anything.

    Property by property

    What each line on the datasheet tells you

    The table below covers the properties you will meet on brick and castable datasheets for steel plants: what each one measures, where it matters in the plant, and what to ask the supplier.

    The properties on a refractory datasheet

    Common ISO test methods are shown for reference. Chinese datasheets usually quote the equivalent GB/T standard; ask which standard each value comes from.

    PropertyWhat it tells youWhere it mattersAsk forCommon ISO test
    Chemistry (Al₂O₃, MgO, C, Fe₂O₃, SiO₂, alkalis)What the brick is made ofEverywhere; impurities such as Fe₂O₃ and alkalis weaken hot performanceMinimum for the main oxide, maximum for impurities; fixed carbon for magnesia carbonISO 12677
    Bulk density (g/cm³)Mass per volume; the same number as tonnes per m³Slag and wear zones, and the tonnage you pay forA minimum, and the price per m³ISO 5017
    Apparent porosity (%)Share of open poresSlag and metal penetrationA maximumISO 5017
    Cold crushing strength (MPa)Strength at room temperatureHandling, installation, abrasionA minimum; never read it as hot strengthISO 10059
    Refractoriness (°C)Temperature at which a test cone bends under its own weightRough ranking onlyNever treat it as the working temperatureISO 528
    Refractoriness under load, RUL (°C)Temperature at which the brick starts to deform under 0.2 MPaLinings that carry load: stoves, roofs, wallsThe deformation level (T0.5, T0.6) and the loadISO 1893
    Creep (%)Slow deformation at a fixed temperature and load over many hoursHot blast stove checkers and domes, years under loadTemperature, load and test durationISO 3187
    Permanent linear change on reheating (%)Lasting shrinkage or growth after reheatingShrinkage opens joints; growth builds stressTemperature and hours of the testISO 2478
    Hot modulus of rupture, HMOR (MPa)Bending strength at high temperatureMagnesia carbon, ladle and converter bricksTest temperature and atmosphereISO 5013
    Thermal shock resistance (cycles)Heating and quenching cycles before failureLadles, stoves, anything that heats and coolsTest temperature and cooling mediumMethod varies; ask which
    Thermal conductivity (W/m·K)How much heat flows throughInsulating and backup liningsThe mean temperature of the testISO 8894
    Castable strength (MPa)Strength after drying and after firingEvery castable liningBoth values, the water addition and the shelf lifeISO 1927

    Worked example

    Reading two real grades side by side

    Look at GZ HA-03 and GZ HA-05 below. Refractoriness is 1790 °C for both. RUL is 1600 °C for both. Creep is 0.5% for both. Read quickly, they look like the same brick with different alumina.

    They are not. HA-03 reaches 0.5% creep at 1400 °C; HA-05 reaches the same 0.5% at 1300 °C. For a hot blast stove zone that runs near 1400 °C under load for years, that one temperature in brackets decides the grade, not the alumina content and not the refractoriness.

    That is the habit to build: read the number, then the condition, then ask which property your zone actually depends on.

    Worked example: two of our low creep high alumina grades

    Exact values from our live library page. Al₂O₃ and density are minimums; Fe₂O₃, porosity, creep and liner change are maximums. Creep at 0.2 MPa.

    GZ gradeAl₂O₃ %Fe₂O₃ %Porosity %DensityCCS MPaRefractoriness °CRUL °CCreep %Liner change %
    GZ HA-03751.5202.760179016000.5 (1400 °C)±0.1 (1500 °C)
    GZ HA-05651.5212.655179016000.5 (1300 °C)±0.1 (1500 °C)

    Where datasheets mislead

    Six ways a weak brick looks strong on paper

    1. Typical values dressed as limits. If the sheet does not say minimum or maximum, ask. A supplier who will not guarantee a value in writing is telling you something.

    2. Refractoriness read as working temperature. A brick with refractoriness above 1700 °C can still deform far below that under load. Use RUL and creep for any lining that carries weight.

    3. Cold strength read as hot strength. A high cold crushing strength says little about how the brick behaves at 1400 °C. For magnesia carbon and other working linings, ask for HMOR at temperature.

    4. The same number at a different condition. As in the example above, an identical creep or liner change figure means nothing until the temperature, load and time match.

    5. Different standards. Values measured to different standards or with different sample shapes are not directly comparable. Ask which standard each value comes from.

    6. A sample that is not the shipment. The datasheet describes what the factory can make. Only a test on samples taken from your shipment tells you what it did make.

    Before you sign

    Five questions to send with every enquiry

    1. Is each value a guaranteed minimum or maximum, or typical?

    2. Which test standard and which test condition (temperature, load, hours) applies to each value?

    3. What are the RUL and creep at my working temperature, and the liner change at my maximum temperature?

    4. What is the dimensional tolerance, and how are the goods packed against moisture?

    5. Will you accept sampling and testing of the shipment before it leaves the factory, against these limits?

    The buying side

    What GZ Visions does for the buyer

    We are a sourcing and inspection company in Shanghai, not a brick factory. Send us the datasheet you have, your vessel and zone, and your working temperature. We read it with you, get the missing limits in writing, check the shipment at the factory before it ships, and arrange third party testing at your request.

    How we work

    What GZ Visions does for your order

    • 01We match the product to your furnace, your temperature and your drawing or list.
    • 02We quote by item and by tonne, FOB China or delivered to your port.
    • 03We check the order at the factory before it ships and can arrange third party testing at your request.
    • 04One contract and one point of contact at GZ Visions.
    • 05Languages: English, Turkish, Portuguese and German from Cengiz; Arabic, Spanish and Chinese through our team.

    FAQ

    Frequently Asked Questions

    What is the difference between refractoriness and refractoriness under load?
    Refractoriness is the temperature at which a test cone of the material bends under its own weight. Refractoriness under load (RUL) is the temperature at which the brick starts to deform under a set load, usually 0.2 MPa. RUL is lower and much closer to how a loaded lining behaves.
    What does creep mean on a refractory datasheet?
    Creep is the slow deformation of a brick held at a fixed temperature and load for many hours, given in %. It matters for linings that carry load for years, such as hot blast stove checkers and domes. Always read it with its temperature, load and test duration.
    What is permanent linear change, or liner change after reheating?
    The lasting shrinkage or growth of a brick after it is reheated to a set temperature for a set time. Shrinkage opens the joints; growth builds stress in the lining. A small value at your maximum temperature is what you want.
    Is cold crushing strength a good measure of brick quality?
    It shows handling and abrasion strength at room temperature, and a very low value is a warning. It does not show how the brick behaves hot. For working linings, ask for hot modulus of rupture at temperature as well.
    What is the difference between typical and guaranteed values?
    A guaranteed value is a limit the whole order must meet: a minimum or a maximum. A typical value is an average and guarantees nothing. Buy against guaranteed limits and test the shipment against them.
    Can GZ Visions check a datasheet I already have?
    Yes. Send the datasheet, the vessel and zone, and the working temperature. A person replies the same business day.

    Request a quote

    Send your drawing or list.

    Furnace type, working temperature, quantities in tonnes and destination port. A person replies the same business day.

    No spam, no list. This reaches the desk directly and is answered by a person.